Stainless acid-resistant steel 1.4429, X2CrNiMoN17-13-3, 1.4406, X2CrNiMoN17-11-2, AISI 316LN, UNS S31653 according to EN 10088-1.
Norma | Gatunek Stali | ||||||||
---|---|---|---|---|---|---|---|---|---|
Skład Chemiczny % | |||||||||
C: | Mn: | Si: | P: | S: | Cr: | Mo: | Ni: | N: | |
EN | 1.4429 - X2CrNiMoN17-13-3 | ||||||||
<0.03 | <2.0 | <1.0 | <0.045 | <0.030 | 16.5 - 18.5 | 2.5 - 3.0 | 11.0 - 14.0 | 0.12 - 0.22 | |
EN | 1.4406 - X2CrNiMoN17-11-2 | ||||||||
<0.03 | <2.0 | <1.0 | <0.045 | <0.030 | 16.5 - 18.5 | 2.0 - 2.5 | 10.0 - 12.5 | 0.12 - 0.22 | |
ASTM | UNS S31653 - AISI 316LN | ||||||||
<0.03 | <2.0 | <1.0 | <0.045 | <0.030 | 16.0 - 18.0 | 2.0 - 3.0 | 10.0 - 14.0 | 0.10 - 0.16 | |
BS | 316S63 - 316 S 63 | ||||||||
<0.03 | <2.0 | <1.0 | <0.045 | <0.030 | 16.5 - 18.5 | 2.5 - 3.0 | 11.5 - 14.5 | 0.12 - 0.22 | |
NF | Z3CND17-12Az - Z 3 CND 17-12 Az | ||||||||
<0.03 | <2.0 | <0.75 | <0.040 | <0.015 | 16.0 - 18.0 | 2.5 - 3.0 | 11.0 - 13.0 | 0.12 - 0.20 |
1.4429, 1.4406, AISI 316LN - specification and application
Austenitic acid-resistant steel resistant to intergranular and crevice corrosion with increased content of Nitrogen and Molybdenum. From standard grades of group 316 it is distinguished by significantly better resistance to chlorides, sea water, acids, cracks and product fatigue during work. In addition, the improved chemical composition allows the material to be used at elevated temperatures in much more aggressive environments than standard 316 steel.
It is used in the production of pump parts, installations and pipelines, parts of radiators, special tanks, heat exchangers, agitators, surgical instruments, prostheses, machine components in the pharmaceutical, chemical, petrochemical, cryogenic, cellulose and food processing industries.
Mechanical properties of 1.4429, X2CrNiMoN17-13-3, AISI 316LN
- Tensile strength, Rm: 580 - 800 MPa
- The yield point, Rp0,2: >280 MPa
- Elongation, A:> 40%
- Modulus of elasticity, E: 220 GPa
- Hardness, HB: <250
- Specific resistance, Ω: 0.75 mkOhm * m
- Impact resistance, KV: > 60J
- Linear expansion coefficient, α: 16.0 * 10-6 K-1
- Thermal conductivity, λ: 15.0 W * m-1 * K-1
- Thermal capacity, cp: 500 J * kg-1 * K-1
Mechanical properties at elevated temperatures
Temperature (℃) | 100 | 150 | 200 | 250 | 300 | 350 | 400 | 450 | 500 | 550 |
---|---|---|---|---|---|---|---|---|---|---|
The yield point, Rp0,2 (MPa) | >211 | >185 | >167 | >155 | >145 | >140 | >135 | >131 | >129 | >127 |
Linear expansion coefficient, α (* 10-6 K-1) | 16.0 | - | 16.5 | - | 17.0 | - | 17.5 | - | 18.0 | - |
Modulus of elasticity, E (GPa) | 194 | - | 186 | - | 179 | - | 172 | - | 165 | - |
Heat treatment
- Supersaturation at 1030 - 1110 ℃ with cooling in water or air
In the above mentioned grades we supply:
- Peeled and drawn bars 1.4429, 1.4406, AISI 316LN, UNS S31653
- Drawn wire 1.4429, 1.4406, AISI 316LN
- Hot-rolled and cold-rolled sheets 1.4429, X2CrNiMoN17-13-3, AISI 316LN, UNS S31653
- Stainless tubes 1.4429, 1.4406, TP316LN
Other grades designations:
X2CrNiMoN17133E, X 2 CrNiMoN 17-13-3, AISI 316 LN, DMV 316 LN, 8MLN, 316S63, 316 S 63, Z3CND17-12Az, Z 3 CND 17-12 Az, 1.4495, UNS S31653, 1.4406, X2CrNiMoN17-11-2.