1.2738, 40CrMnNiMo8-6-4, AISI P20+Ni, 40CMND8 - plastic mould steel, data according to ISO 4957:2001

Standard Grade
Chemical composition %
C: Si: Mn: P: S: Cr: Mo: Ni:
ISO 1.2738/40CrMnNiMo8-6-4
0.35 - 0.45 0.2 - 0.4 1.3- 1.6 <0.03 <0.03 1.8 - 2.1 0.15 - 0.25 0.9-1.2
GOST 40Ch2GNM - 40X2ГHM
0.35 - 0.45 0.2-0.4 1.3-1.6 <0.035 <0.035 1.8-2.1 0.15 - 0.25 0.9-1.2
ASTM AISI P20+Ni
0.4 - 1.5 - - 1.9 0.2 1.0
NF 40CMND8
0.4 0.3 1.5 <0.012 <0.005 1.9 0.2 1.0

1.2738, 40CrMnNiMo8-6-4, AISI P20+Ni, 40CMND8 – description

1.2738 is a plastic mould tool steel, used mainly for plastic injection die moulds. It can be viewed as enhanced version of 1.2311 alloy, with 1% nickel content having a positive effect on hardenability.

The steel is machinable, polishable, and suitable for texturing. Welding is somewhat difficult, but possible. Make sure to pre-heat and perform tempering, when the piece colled down after welding.


Physical and mechanical properties

1.2738 - general physical and mechanical properties in ambient temperature:

  • Linear expansion coefficient: 11.2 *10-6m/(m*K)
  • Thermal conductivity: 35 W/(m*K)
  • Hardness (in soft annealed condition): < 235 HB
  • Hardness (in hardened and tempered condition): < 51 HRC

Linear expansion coefficient of 1.2738 steel, in high temperature and in hardened and tempered condition:

  • Temperature range: 20-200 °C - 12.8 *10-6m/(m*K)
  • Temperature range: 20-300 °C - 13.5 *10-6m/(m*K)
  • Temperature range: 20-500 °C - 14.3 *10-6m/(m*K)
  • Temperature range: 20-700 °C - 14.9 *10-6m/(m*K)

Thermal conductivity of 1.2738 steel, in high temperature and in hardened and tempered condition:

  • Testing temperature: 350 °C - 34 W/(m*K)
  • Testing temperature: 700 °C - 33 W/(m*K)

Hardness of steel 1.2738 in hardened and tempered condition, at various tempering temperatures:

  • Tempering temperature: 100 °C - 51.5 HRC
  • Tempering temperature: 200 °C - 50.2 HRC
  • Tempering temperature: 300 °C - 48 HRC
  • Tempering temperature: 400 °C - 46.2 HRC
  • Tempering temperature: 500 °C - 43 HRC
  • Tempering temperature: 600 °C - 39 HRC
  • Tempering temperature: 700 °C - 29 HRC

Heat treatment and working

Recommended working and heat treatment parameters for 1.2738 alloy:

  • Forging: 1050-850 °C
  • Rolling: 1050-850 °C
  • Quenching: 840-870 °C
  • Soft annealing: 710-740 °C

We deliver this steel alloy as:

  • Forgings
  • Rods

Replacements, equivalents and other designations:

1.2738, 40CrMnNiMo8-6-4, AISI P20+Ni, 40CMND8, 40Ch2GNM, 40Х2ГНМ, M238


THIS WEBSITE USES COOKIES TO IMPROVE AND FACILITATE YOUR ACCESS TO THE WEBSITE AND TO KEEP STATISTICS. IF YOU CONTINUE TO USE THIS SITE, YOU AGREE THAT THE COOKIES WILL BE STORED ON YOUR DEVICE
PRIVACY POLICY
How do I disable cookies
AGREE